Metal JBK-75 - testing conditions (record 6)
- Creators
- HMB, Admin
Description
Metal Type: JBK-75
Corrosion
No Data
External Conditions
No Data
Fracture/Fatigue Mechanics
Tensile Yield Strength: 793MPa
UTS Change: 1.42%
Ultimate Tensile Strength: 1207MPa
Reduction Area: 56.3%
Engineering Strain Fracture:: 0.331
Hydrogen Properties
External Hydrogen Exposure: Charged then tested in air (No)
Internal Hydrogen Exposure: Tested in H2 (Yes)
Material Dimensions
Size of Material (coupon, pipe): 20mm diameter bar
Shape: Machined Round
Dimensions: 5mm Diameter, 25mm Guage Length
Testing Conditions (Pressure)
10000000Pa
Testing Conditions (Temperature)
Temperature (Constant) 153K
Welding
No Data
Other Properties
History of Use: Hot-rolled stock, solution treated at 1253K for 1 h, water quenched, aged 8 h at 1013 K & air cooled.
Manufacturer: Institute of Metal Research, Shenyang, China